SPECIFICATION OF COLD ROLLED NON-ORIENTED ELECTRICAL STEEL
 

Grade

 

Thickness

 

Assumed Density

Max. core loss

Typical Core Loss (W/kg)

Induction

Min.

Lamination

factor

W/kg

mm

 ( kg/dm3)

50Hz

50Hz

 

 

1.0T

1.5T

1.0T

1.5T

5000A/m

 %

B35A440

0.35

7.70

1.80

4.40

1.69

3.89

1.64

95

B35A550

7.75

2.25

5.50

1.70

3.90

1.66

B50A470

0.5

7.70

2.00

4.70

1.77

4.07

1.62

97

B50A600

7.75

2.60

6.00

1.85

4.28

1.65

B50A700

7.80

3.00

7.00

2.58

5.51

1.68

B50A800

7.80

3.60

8.00

2.68

5.84

1.68

B50A1000

7.85

4.40

10.00

2.98

6.51

1.69

B50A1300

7.85

5.80

13.00

3.25

7.11

1.69

B65A600

0.65

7.75

2.70

6.00

2.09

4.78

1.64

97

B65A700

7.75

3.15

7.00

2.31

5.25

1.65

B65A800

7.80

3.60

8.00

2.87

6.19

1.66

B65A1000

7.80

4.40

10.00

3.14

6.97

1.68

B65A1300

7.85

5.80

13.00

3.54

8.01

1.69

B65A1600

7.85

7.10

16.00

4.18

9.52

1.69

 
 
 
 
 
 
l5